T1 Tool Steel | SKH2 | 2750 | W18Cr4V | HS 18-0-1 | 1.3355 High Speed Steel
AISI T1 Tool Steel is typical W High Speed Steel. HSS T1 is the most widely used tungsten type of high speed steel, high temperature hardness and red hardness is high, easy to grinding. ASTM T1 applicable for working temperature below 600 ℃ can still keep the cutting performance of cutting tools, such as vehicles, shaver, milling, reaming, broach, drilling, gear cutting tools and tap, die, etc We supply T1 high Speed tool steel in round bar, flat, square bar, plate,sheet.
Supply Form of HSS T1 Tool Steel -ASTM A681 High Speed Steel
Supply Range of SAE T1 Tool Steel HSS Tungsten High Speed Steel
T1 Steel Round Bar: diameter 1mm – 400mm
T1 Steel Plate: thickness 1 –500mm x width 200– 1400mm
T1 Steel Block: 210mm x 500-810mm
Chemical Composition of T1 Tool Steel Material
ASTM A681 | C | Si | Mn | P | S | Cr | Mo | V | w |
T1/ T12001 | 0.65~0.80 | 0.20~0.40 | 0.10~0.40 | 0.030 Max | 0.030 Max | 3.75~4.50 | – | 0.90~1.30 | 17.25~18.75 |
DIN 17350 | C | Si | Mn | P | S | Cr | Mo | V | w |
1.3355/HS 18-0-1 | 0.70~0.78 | ≤0.45 | ≤0.40 | 0.030 Max | 0.030 Max | 3.80~4.50 | – | 1.00~1.20 | 17.50~18.50 |
GB/T 9943 | C | Si | Mn | P | S | Cr | Mo | V | w |
W18Cr4V | 0.70~0.80 | 0.20~0.40 | 0.10~0.40 | 0.030 Max | 0.030 Max | 3.80~4.40 | <0.30 | 1.00~1.40 | 17.5~19.00 |
JIS G4403 | C | Si | Mn | P | S | Cr | Mo | V | w |
SKH2 | 0.73~0.83 | ≤0.45 | ≤0.40 | 0.030 Max | 0.030 Max | 3.80~4.50 | – | 1.00~1.20 | 17.20~18.70 |
AISI T1 Tool Steel Material Equivalent and Related Speciations
USA | German | Japan | China | ISO |
ASTM A681 | DIN 17350 | JIS G4403 | GB/T 9943 | ISO 4957 |
T1 | 1.3355 | SKH2 | W18Cr4V | HS 18-0-1 |
SAE T1 Tool Steel Material Mechanical Properties
Hardness, Rockwell C (tempered at 621°C, quenched at 1277°C): 63-65 HRc.
Elastic modulus: 190-210 GPa
SAE T1 Tool Steel Physical Properties
Density: 8.67kg/cm3
Thermal expansion: 9.7 x 10-6/°C at 20-200°C more
Forged of T1 HSS Steel metal material
Pre-Heating to 650-750℃,Then heat to forged temperature. Soak at 1204°C, ensure heat thorough. Then start forged, the forged temperature no low than 950℃. After forging, cool slowly.
Heat Treatment of SAE T1 Steel-A681 High Speed Tool Steel
- T1 HSS Steel Annealing
Slowly heat to 816-871℃,then slowly Cool to 538℃(1000℉) in heat treatment furnace. Then cool in air. After annealing hardness HBS: 255 Max
- T1 tool Steel Hardening
T1 steel having very high hardenability and should be hardened by cooling in still air. The use of a salt bath or controlled atmosphere furnace is desirable to minimize decarburization, and if not available, pack hardening in spent pitch coke is suggested.
- Quenching of HSS T1 Tool Steel material
Quenching temperature / ℃ | salt bath furnace: 1277
Quenching temperature / ℃ | controlled atmosphere furnace: 1288
The heat preservation time/min: 5 ~ 15
Quenching medium: Oil cooling
Hardness: 63 HRc Min
- Tempering Of HSS T1 Tool Steel
Tempering temperature / ℃ : 540-564
After tempering hardness HRC or higher: 63 Min
Application of Sae T1 tool Steel ASTM HSS
AISI T1 high speed tool steel is the most widely used tungsten is a general type of high speed steel, high temperature hardness and red hardness and hardness is high, easy to grinding. Apply for working temperature below 600 ℃ can still keep the cutting performance of cutting tools, such as vehicles, shaver, milling, reaming, broach, drilling, gear cutting tools and tap, die, etc., suitable for processing soft or medium hardness material below (300 ~ 320 hb). And the production of high temperature abrasion machine
Quality Assured of Sae T1 Tool Steel
Quality assured by ISO 9001:2008 quality management system. Our all T1 tool steel all had by SEP 1921-84 ultrasonic inspection (UT Test). Quality Grade: E/e, D/d, C/c.